Sunday, 28 May 2017

Cast Iron Step Repair

This is a broken Cast Iron landing step for an old spiral staircase.




 Edges of the crack ground out to a "vee".

 First attempt at welding - stick welded using Nickel based rods. Pretty horrible - old rods, possibly wrong power setting, out of practice & even though these rods are meant for "cold" welding, it probably would have come out a lot better if the casting had been pre-heated.

 After grinding out a lot of the Nickel stick welding, I tried again, this time TIG welding using Phosphor Bronze rods.

 The welds on the under side were left.

 The ones on top ground smooth

Ready to be sanded all over before re-painting.

Tuesday, 1 February 2011

Special inlet manifold/plenum chamber for an Escort Turbo engine fitted in a Kit Car

Our customer had fitted a Ford Escort Turbo engine into a Caterham/Lotus 7 type of kit car. The original inlet manifold for the transverse mounting in the Escort wasn't suitable for the inline orientation in the kit car, so a new, or rather radically modified, manifold was needed.
This was a fairly straightforward aluminium welding job. The customer brought us the large aluminium tube already cut to size & with holes cut where the (already cut down) inlet manifold needed to be attached.



We then had to weld on a disc at each end of the tube - at one end a blanking plate with a threaded hole for a sensor

and at the other end, one to take the throttle body.


This shows the throttle body mounted in position.

Friday, 24 December 2010

Twin Disc conversion for Triumph Trident

First step was to machine the caliper bracket from a suitable aluminium billet.

A flat was milled on the fork leg.

The bracked was placed in position on the fork leg & held with two small tack welds.

 Followed by a larger tack on the back of the bracket.


The bracket was fully welded to the fork leg on both sides & the welds were smoothed, blended & lightly polished. Then a bracing rib was added.
The finished fork leg after final smoothing, blending & light polishing of the welds and drilling & tapping the holes for the caliper bolts. New one on the right, original on the left.

Brake Caliper Bracket for twin disc brakes on Triumph Trident

Wednesday, 21 July 2010

Kawasaki ZX Motorcycle Frame

This Alloy motorcycle frame was brought to us when the customer, having taken the engine out, noticed that the box section rear cross member wasn't actually fixed to the main frame. It seemed as if the weld had cracked. However, when we ground the metal away to provide a good chamfer for re-welding, we found that the cross member was anodised where it entered into the side part of the frame. It appears that it was never properly welded in the first place! With the engine installed, the engine mounting bolts held everything together so the fault never became apparent until the engine was taken out.








Not the neatest of welds but good & strong & definitely joining both parts together!


Sunday, 27 June 2010

Cracked Gearbox - disaster!

This was a Ford Escort gearbox which had been cracked underneath & was leaking oil. It was brought to us complete (just the gearbox, not the whole car!) & still with oil in it
Could we weld it up?.......
One problem was that we didn't know how thick the casing was so couldn't run the risk of using too much power & burning a hole through the casing & couldn't grind out the cracks for fear of going through. That exacerbated the main problem, that the cracks were dirty/oily & that though the outside of the casing can be cleaned, the inside of the casing was still oily. Welding over the cracks just drew the dirt & oil out & contaminated the weld.



This can be seen here as sooty discolouration & holes in the weld.





















Sometimes you can get away with it by cleaning the surface again & grinding the weld off and going over it again. The "dirt" floats to the top of
the weld pool so it gets removed when you grind the weld off (in theory - if it's not too bad).








In this case, the contamination just kept coming through.
















The weld continues to grow & still keeps cracking.








The final complete mess! Full of holes & craters. Still cracked, still leaking - a complete waste of time.
The correct way to do this would have been to strip the gearbox completely so that the casing could be thoroughly cleaned inside & out, the cracks could be ground out to remove any dirt/old oil in them & it could be welded on both sides to ensure a good weld. Then rebuild the gearbox.
But that would have cost more than buying a secondhand gearbox, which is what the customer ended up doing & we should have told him to do in the first place!
You live & learn.

Tuesday, 22 June 2010

Air Conditioning Pipe

This pipe is from an air conditioning system on a car. The engine mounts had collapsed & allowed a pulley to contact the pipe & wear it away. When brought to us, only a pinhole was visible in the damaged area, but a poke with a scriber soon revealed how much of the aluminium was worn away & not just dented.







Even if the problem had been just a tiny pinhole, the repair would have been done the same way:-
Cut a little patch from sheet aluminium & TIG weld it in position all around the damaged area.
Trying to weld over the hole just vapourises the fluid remaining in the pipe which then contaminates the weld. Using a patch gives a much better chance of getting a good weld with no pinholes (& leaks). Even so, extraction is needed to suck away the fumes that come out of the end of the pipe & in this case, the rubber hose which is clipped to the aluminium pipe was put into a tub of water to keep it cool while the welding was being done.